Joint efficiency and radiography (UW-11, UW-12)
Joint efficiency (E) is the factor ASME Section VIII Division 1 applies to a welded joint in the thickness formulas. It depends on the joint type and how much it is radiographed: a double-welded butt joint is 1.0 with full radiography, 0.85 with spot radiography and 0.70 with none (Table UW-12). Less radiography means a thicker shell.
Pujan Motiwala · Written to the ASME BPVC 2025 Edition · checked against ASME's and the National Board's public pages on

Video chapters (10)
- 0:00What ASME Joint Efficiency (E) & Table UW-12 Do
- 0:21Joint Type (1–8 Form) vs. Joint Category (A–D Location — UW-3)
- 0:42Table UW-12 Values: Type 1 (1.00 / 0.85 / 0.70), Type 2 & Type 3
- 1:024 Mandatory Full-RT Triggers Under UW-11(a) (Lethal, 1-1/4 in, 50 psi)
- 1:22Worked 48 in Shell Example: 5/16 in vs. 3/8 in vs. 7/16 in Plate
- 1:44Seamless Shells (UW-12(d)), Intersecting B/C Seams & UW-51 / UW-52
- 2:04Official Scope Citations (Sec VIII Div. 1, Sec I Part PW & Sec V)
- 2:26Comparing Design E Against Actual Weld Map RT in Boiler ERP
- 2:462025 Edition Notice & Authorized Inspector Verification
- 3:00Next Steps: Vessel Heads (S29), Shell Thickness (S03) & Section V (S12)
What is joint efficiency in ASME Section VIII?
Joint efficiency (E) is the factor Division 1 applies to a welded joint in the thickness formulas, set by the joint type and how much of it is radiographed (Table UW-12, 2025 Edition). It goes straight into the shell thickness and head formulas, so a lower E means a thicker wall. The Code text is ASME's and paid; this guide cites paragraphs.
What are the joint efficiency values?
For the common butt joints, from Table UW-12:
| Joint type | Description | Full radiography | Spot radiography | None |
|---|---|---|---|---|
| 1 | Double-welded butt joint, or equivalent full penetration | 1.00 | 0.85 | 0.70 |
| 2 | Single-welded butt joint with a backing strip left in | 0.90 | 0.80 | 0.65 |
| 3 | Single-welded butt joint without backing | – | – | 0.60 |
Lap and fillet joints (Types 4 to 6 and others) have lower values again and are limited in where they may be used.
What is the difference between joint type and joint category?
Type is what the joint is (its form, Types 1 to 8); category is where it sits (A to D), because location decides how much stress it carries:
- Category A: longitudinal welds in shells and nozzles, and the weld joining a hemispherical head to the shell. They carry the hoop stress, the higher one.
- Category B: circumferential welds between shell courses and between the shell and most formed heads.
- Category C: welds attaching flanges, tubesheets and flat heads.
- Category D: welds attaching nozzles and communicating chambers.
Both go on the data report.
When is full radiography mandatory?
UW-11(a) makes full radiography of butt welds mandatory in several cases, among them:
- vessels in lethal service;
- butt welds thicker than the limit for the material (for P-No. 1 carbon steel, 1¼ in, 32 mm);
- unfired steam boilers with a design pressure above 50 psi (3.4 bar);
- wherever the designer has taken the full-radiography efficiency (E = 1.0 for a Type 1 joint).
Otherwise the choice is the designer's, and it is commercial: full radiography costs more in examination and saves steel.
How much thicker does a shell get with less radiography?
Take a 48 in inside diameter shell at 150 psi, S = 20,000 psi, corrosion allowance 0.125 in, Type 1 longitudinal joints:
| Radiography | E | Hoop thickness | With corrosion | Plate |
|---|---|---|---|---|
| Full | 1.00 | 3,618.75 / 19,910 = 0.182 in | 0.307 in | 5/16 in or ⅜ in |
| Spot | 0.85 | 3,618.75 / 16,910 = 0.214 in | 0.339 in | ⅜ in |
| None | 0.70 | 3,618.75 / 13,910 = 0.260 in | 0.385 in | 7/16 in |
The shell calculator takes a separate E for the circumferential joints, which govern the longitudinal-stress check.
What joint efficiency does a seamless shell or head get?
A seamless part has no longitudinal joint, but its E still depends on the circumferential welds joining it: with those spot radiographed to the rule for this case (UW-11(a)(5)(b)), a seamless part uses E = 1.0; without, 0.85 (UW-12(d)).
Does full radiography of the long seams need anything else?
Yes: to take E = 1.0 on Category A joints, the Category B and C butt joints that intersect them must at least be spot radiographed (UW-11(a)(5)(b)). That is why designers often specify "full RT of Category A, spot of Category B".
Who sets the radiography method and acceptance?
The method comes from Section V, which ASME describes as its NDE standards; acceptance comes from Division 1: UW-51 for full radiography and UW-52 for spot. Division 1 also allows ultrasonic examination in place of radiography in defined cases; check your 2025 book for the conditions.
When does joint efficiency apply at all?
To Section VIII Division 1 vessels, which ASME describes as covering "pressure vessels operating over 15 psig, fired/unfired". Section I boilers have their own weld rules in Part PW.
What does our software keep for joint efficiency?
Our US boiler demo's weld map records each seam's category (A, B or D), joint type, WPS, welder stamps, NDE method (RT spot or full, UT, MT) and report, and prints it in the job's ASME record package, so the E on the calculation and the radiography actually done can be compared. See ERP for boiler and pressure vessel shops.
Quoted from the official text (1)
“ASME BPVC Section VIII Division 1 provides design, fabrication, inspection, testing & certification rules for pressure vessels operating over 15 psig, fired/unfired.”
ASME Section VIII Division 1 product page, description
WPS and PQR registers, welder continuity, heat numbers from receipt to nameplate, and the data report package: the records a Code shop keeps, in one system.
A boiler manufacturer's system, from enquiry to dispatch and the IBR folder, with sample logins: try the live demo.
A boiler and pressure vessel shop's system, from inquiry to shipping and the ASME data report package, with sample logins: try the live demo. Fixed price, scope agreed before work starts: see the prices.
Official sources
- Boiler and Pressure Vessel Certification. ASME, November 1, 2026.
- BPVC Section VIII Division 1 (2025). ASME, July 1, 2025.
- BPVC Section V: Nondestructive Examination (2025). ASME, July 1, 2025.
What this page is not
A guide written by Ahrom Labs, not engineering advice, and not yet reviewed by an Authorized Inspector. The ASME Code is copyrighted and sold by ASME: paragraphs are cited by number and explained in our own words, never reproduced. Check every figure against your copy of the 2025 Edition and with your Authorized Inspector before relying on it. Last updated .
Talk to us about your systems.
Tell us what's held together with workarounds right now. We reply to every message ourselves.